KEXIN · Technical Notes
TECHNICAL NOTE · FINISHING

Surface Finishes: What Works on Which Alloy

Kexin Engineering · Updated 2026-11-14 · 8 min read

Finishing is where most cosmetic rejects originate, and it is usually the one process the die caster does not own. The choice of finish is also decided by the alloy long before anyone picks up a spray gun — which is why the wrong finish on the right casting produces a project that neither supplier can fix.

1. The short decision table

FinishZincAluminum die castNotes
Electroplating (Cu/Ni/Cr)Excellent — the standard routePossible but demanding; rarely chosenZinc takes a true mirror finish. Aluminum's silicon content makes pretreatment fussy and consistency poor.
Electroless nickelGoodGoodEven coverage including internal surfaces; common for EMI continuity on housings.
Powder coatingWorkableExcellentThick (60–120 µm), hides surface detail, good corrosion barrier. Needs a conductive substrate and a temperature the part can survive.
Wet paintGoodGoodThinner (20–40 µm), cheaper at low volume, more colour flexibility for small batches.
AnodisingNot applicableNot cosmetic on high-silicon die castSee §5 — the silicon does not anodise, so the result is dark and blotchy.
Bead blasting / tumblingGoodGoodA preparation step or a final finish for industrial parts. Uniformity depends on part geometry.
Passivation / conversion coatGoodGoodBare corrosion protection and a paint base. Not decorative.
Bare, as-castPoor outdoorsModerate outdoorsZinc oxidises to a white corrosion product; aluminum forms a protective oxide but stains.

2. Plating on zinc: the manufacturing sequence matters

A chrome-plated zinc casting is not simply "dipped". The sequence is: polishing to remove casting skin and flow marks → degreasing → acid activation → copper strike → copper build → nickel → chromium. Each layer has a purpose, and each one can fail independently.

The practical consequence: plating quality is decided by the polish, not by the plating bath. A casting with flow marks, cold shuts or visible porosity will show every one of them after plating, magnified. This is why plating and casting cannot be sourced separately without an argument over who owns the defect.

3. The thickness window, and why it is a window

LayerTypical thicknessWhat happens if too thinWhat happens if too thick
Copper15–30 µmCannot level the casting surface; roughness telegraphs throughCost, and stress build-up causing blistering
Nickel10–20 µmCorrosion resistance and salt spray hours drop sharplyInternal stress, cracking on flexing parts
Chromium0.1–0.5 µmWear resistance and colour depth lostMicro-cracking, and a bluish cast on some baths

When a customer specifies "chrome plated", ask for the layer stack and thicknesses. A supplier who cannot state them is either subcontracting without specification or does not know — and either way the salt spray result will be a surprise.

4. Powder coating and painting: where the casting fights back

Both processes need a clean, conductive, slightly rough surface. Die castings give you three challenges:

Powder coating is thicker and more durable but hides fine detail and needs a cure temperature — check the alloy and any plastic inserts first. Wet paint is thinner and cheaper for small batches, and lets you match a colour more easily.

5. Why anodised die-cast aluminum is usually a mistake

The mechanism: anodising grows an oxide layer from the aluminum in the alloy. The silicon in A380, A383 and ADC12 — 8 to 11% of the alloy — does not anodise. It stays as silicon particles while the aluminum around it converts to oxide, so the coating is discontinuous and the surface reads dark, mottled and matte.

The result is not a cosmetic finish. On a hidden internal part it may be acceptable as a corrosion measure; on a visible housing it is a reject.

If a specification genuinely requires anodised aluminum, the part usually needs to be extruded or machined from a low-silicon wrought alloy (6061, 6063), not die cast. That is a different manufacturing route with a different cost structure. It should be identified at the quoting stage, not after the tool is cut.

6. How to write a finish specification that can be enforced

  1. Name the process and the layer stack — not just "chrome". Example: copper 20 µm / bright nickel 15 µm / chromium 0.3 µm.
  2. State the acceptance test and the standard — adhesion by cross-hatch or thermal cycling, thickness by X-ray or coulometric method, corrosion by neutral salt spray hours.
  3. Set a salt spray target that fits the market. Indoor hardware and outdoor architectural fittings are not the same requirement, and the price difference is real.
  4. Define the cosmetic grade per face. Which surfaces must be flawless, which may carry a flow mark, which are hidden.
  5. Define porosity acceptance before finishing. A machined or plated face that reveals porosity is a casting issue, and the acceptance limit has to be agreed while the parts are still bare.
  6. Name who inspects and who pays. If finishing is subcontracted, the die caster still owns the result in the customer's eyes. Write that responsibility down.

7. How we handle finishing

Castings are made in-house; plating and anodising run through qualified partners against our specification, and we inspect the finished parts before they ship. That means one commercial counterparty for you and one technical owner for the process chain — if a lot fails salt spray, the argument happens inside our supply chain rather than across yours.

We ship the finish test data with the lot: layer thickness readings and the salt spray or adhesion result, as applicable. If a customer's specification requires a particular standard or a particular laboratory, tell us at the quote stage so it is priced and planned rather than discovered at shipment.

Need a finish recommendation?

Tell us the alloy, the environment and the cosmetic requirement — we will tell you which finishes are viable and which are not.

WhatsApp Email us