A drawing that says "±0.02" in the general tolerance block is not a precise drawing. It is a drawing that has not decided what matters — and the supplier will price it as though every surface were critical, because that is what the words require. This note explains what the published tolerance systems actually cover, where the boundary between as-cast and machined accuracy sits, and how to write a block that can be met.
1. Three separate things that drawings confuse
- Dimensional tolerance — how far a length may deviate. This is what tolerances tables in standards describe.
- Geometric tolerance — flatness, parallelism, position, profile. Separate from size, and usually the actual limiting factor on a casting.
- Surface condition — roughness, porosity acceptance, cosmetic grade. Not a tolerance at all, but frequently the reason a part is rejected.
A tolerance block that addresses only the first of these will be met while the parts are still unusable. Most rejection arguments we have with first-time buyers are about the second and third, which were never written down.
2. The published systems, and what they are for
ISO 8062 — general tolerances for castings
ISO 8062 defines dimensional tolerance grades (typically DCTG 1 to DCTG 16) and machining allowance grades for castings generally. Higher grade numbers mean coarser tolerance. The standard is a framework: it gives you a way to state a grade and look up an expected deviation band for a given nominal size, rather than writing a number on every dimension.
For die castings, the practical range is at the fine end of the table. An as-cast die casting is a much more accurate process than sand casting, and a drawing that selects a sand-casting grade for a die-cast part is specifying something the process will beat easily — which sounds good and is actually harmless. The problem is the reverse: selecting the finest grade in the table and assuming the die caster will hit it without a machining operation.
DIN 1686 / DIN 1688 — German die casting standards
The DIN 1686 system is the reference most European die casters quote against. It separates tolerances for dimensions formed within one mould half from those spanning the parting plane, and separates again for dimensions affected by moving parts (slides, ejectors). That distinction matters more than the raw numbers: a dimension across a parting line has inherently more variation than one inside a single cavity half, because it depends on the die closing repeatably.
NADCA — North American Die Casting Association
NADCA publishes product standards that give precision tolerance bands separately for zinc and aluminum, and also standard tolerances for features like flatness, draft, and cored holes. NADCA's zinc bands are tighter than aluminum, which matches the physics: zinc is cast at roughly 400 °C rather than 680 °C, so there is less thermal contraction, less die growth and less distortion.
Use these as bands, not as claims. Every standard's tolerance tables assume a part of reasonable size and shape, cast in a production tool that has been properly developed. They do not promise that any arbitrary geometry will hit any specific grade. When we quote a tolerance, we quote against the feature — not against a table row — and we say so if we think a particular feature cannot hold it.
3. The ranges we actually work to
The numbers below are the working ranges we quote against for normal production parts. They are not a substitute for the standards; they are what those standards translate to on a shop floor for parts in the sizes we normally run.
| Feature | Zinc alloy, as-cast | Aluminum, as-cast |
| Small dimensions, same die half (under 25 mm) | ≈ ±0.025 mm | ≈ ±0.05 mm |
| Medium dimensions, same die half (25–100 mm) | ≈ ±0.05 mm | ≈ ±0.08 mm |
| Dimensions across the parting line | ≈ ±0.08 mm, add size effect | ≈ ±0.12 mm, add size effect |
| Dimensions affected by a slide or moving core | add ≈ 0.05 mm to the above | add ≈ 0.08 mm to the above |
| Straightness / flatness, per 25 mm | ≈ 0.02 mm | ≈ 0.03 mm |
| Draft, external wall | 1° minimum, 2° preferred | 1.5° minimum, 2–3° preferred |
| Minimum cored hole diameter | ≈ 1.5 mm | ≈ 2.5 mm |
| Cast thread, coarse pitch | workable to ≈ 2× diameter depth | prefer machined |
| After CNC, machined features | ±0.02 mm routine, ±0.01 mm on request | ±0.02 mm routine, ±0.01 mm on request |
| After CNC, geometric (flatness / position) | 0.01–0.02 mm | 0.01–0.02 mm |
The last two rows are the point of the whole article. As-cast accuracy and machined accuracy differ by roughly a factor of two to three. A drawing that needs ±0.01 mm on a bore is asking for a machining operation, and pricing it as-cast is how a quote ends up wrong in either direction — too cheap to deliver, or too expensive to win.
4. Where as-cast tolerance comes from, physically
It is worth understanding why the numbers are what they are, because then the quoted figure stops looking arbitrary:
- Shrinkage compensation. The die cavity is cut oversize by the alloy's shrinkage factor (roughly 0.4–0.6% for zinc, 0.5–0.7% for aluminum). That factor is not perfectly constant across a part with varying wall thickness, so the compensation is a compromise. Local variation shows up as dimensional scatter.
- Die thermal growth. The die is hot and expands. Temperature distribution across the die is not perfectly uniform, so different regions expand differently — and the pattern shifts with cycle time.
- Die wear and erosion. Over a tool's life, gates erode and corners round off. The part produced at shot 400,000 is not the part produced at shot 4,000. A tolerance that is just barely met at first article may be lost by mid-life; a good tool design budgets for this.
- Parting-plane repeatability. This is why cross-parting-line dimensions carry extra allowance: the die must close to the same position every cycle, and the mechanism has clearance.
- Moving cores and slides. Each moving element adds its own clearance and wear to the stack, so a feature formed by a slide is inherently less repeatable than one formed by the cavity block.
- Ejection distortion. A thin part pushed off by ejector pins can flex slightly and stay flexed. Flatness suffers before dimensions do.
None of these are defects. They are the process. A drawing that ignores them becomes a source of permanent concession notes.
5. Writing a tolerance block that can be met
- State a general tolerance for the bulk of the part. Something coarser than you think you need is usually right — most surfaces are not functional. This is where the cost is controlled.
- Call out critical dimensions individually. Typically four to eight features: bores that take a bearing or a shaft, faces that mate, latch engagement points, connector interfaces.
- Separate as-cast from machined. Mark which features are produced as-cast and which will be machined. If a dimension is on a machined face, say so and give the datum.
- Define the datum scheme explicitly. A positional tolerance without a datum reference cannot be inspected and cannot be argued about — it just becomes a rejection.
- Specify geometric tolerance where it actually limits the part. Flatness on a sealing face, position on a bore pattern, profile on a mating surface. Not "everything, everywhere".
- Write the cosmetic and porosity acceptance criteria. Which faces are A-surface, what porosity is acceptable on a machined face, whether flow marks are rejects. This is a separate clause from tolerance and it prevents the most common end-of-project dispute.
- Say what happens at the boundary. If a dimension is at the limit, is it accepted or rejected? Define the measurement method and the gauge, because two people measuring the same part with different methods will disagree.
6. The three tolerance mistakes we see most
"±0.02 general." This is the single most common entry in a first drawing we receive, usually inherited from a CNC-machined prototype. On a die casting it prices every surface as critical and is not achievable as-cast on most of them. It converts a straightforward job into a permanent deviation-request conversation. Write ±0.10 general and tighten the six features that matter.
Position tolerance with no datum. "True position 0.1" with no A/B/C reference is not a specification — it is a hope. It cannot be measured, so it gets measured inconsistently, and the argument is about the measurement rather than the part.
Tolerance carried over from a machined part. If the previous version of the part was CNC-machined from billet, every dimension could be held to ±0.02 at no extra cost, because machining holds what it holds. Die casting does not work that way: accuracy is bought in steps — as-cast, then fixtured machining, then fine machining. Ask what each step costs before writing the drawing.
7. How we handle tolerance in a quote
When a drawing arrives, we read the tolerance block before the geometry, because it determines whether the part is a casting job or a casting-plus-machining job. The reply states which features we propose to cast, which to machine, what accuracy each will hold, and which tolerances on the drawing we believe should move.
If a tolerance on your drawing is tighter than the process needs, we will say so and quote the looser version alongside. If it is tighter than the process can hold and the function genuinely requires it, the honest answer is a machining operation — and that answer belongs in the quote, not in the first rejected lot.
Send a drawing, get the tolerance read back.We will tell you which features we can cast to size and which need machining — before you commit to a tool.
WhatsApp
Email us